Surface Replication Compounds

The first challenge when measuring a surface topography via optical techniques is getting the sample to the lab. Although optical surface roughness measurement does not damage the component per se (NDT), the fact of fitting it into a microscope generally requires the destruction of the original component. The surface replication compounds solve this issue.

IMG_0006

The surface replication technique has been used in aerospace, industrial and nuclear applications for many years, particularly for in-situ high resolution metallography. The replica technique allows reproducing a mirrored topography of a surface into a reduced dimensions polymeric sample. This technique also allows taking measurements on the exact same spot before and after running so the surfaces can accurately be compared afterwards. This is extremely useful when assessing wear phenomena.

 

Surface Replication Kit

Surface replication compounds suppliers generally provide a kit to obtain surface replicas with the following instruments:

  1. Dispensing pistol
  2. Compound cartridge
  3. Several disposable mixing nozzles

IMG_0056

The cartridge is mounted on the dispensing pistol and the mixing nozzle is attached to the other end of the cartridge. The trigger of the pistol mechanically pushes the plunger of the cartridge squeezing out the replication compound into the mixing nozzle. The compound flows through the nozzle until its released to ambient over the desired surface.

Working Principle

The idea behind is quite simple:

  1. The fast-curing viscous polymer is applied on the desired surface.
  2. Once the replication compound is dry, it is carefully peeled off from the original surface. The original component surface roughness is captured on the polymer surface without damaging it.
  3. The high-resolution elastomeric replica of the surface can be easily studied in the lab afterwards.

The cartridge contains a specially formulated two-part silicon rubber. When these semi-viscous liquids are pushed out of the cartridge and mixed in the nozzle its curing begins. The compound must be pushed through the nozzle and applied on the surfaces before it solidifies. Since the two polymers are not mixed until reaching the nozzle those are kept inside the cartridge without risk of vulcanization.

IMG_0050

The particularly-shaped nozzle is used to properly mix the polymers so the compounds begin to vulcanize in it. Because of that the mixing nozzle is disposable and needs to be replaced for every set of measurements. It is then advised to previously prepare all the surfaces for measurement so the compound can be applied to all of them using a single nozzle.

 

Surface Preparation before applying the Replication Compound

It is recommended to previously clean and dry the surfaces to measure. This way the compound will output its best results. The selection of the cleaning solvent will depend on the original surface characteristics. The silicon compounds is highly inert, it is suggested to contact the compound manufacturer when using a special cleaning solvent.

 

Difference between Replication Compounds

There is a wide range of replication compounds available specially tailored to the surface and environment characteristics. The temperature at which the compound is applied, for example, plays an important role since this will directly impact the curing time of the polymer.

The different compounds mainly approach the following issues:

      1. Viscosity: A higher viscosity fluid is needed when measuring on a tilted surface or when facing a strong gas flow; otherwise the compound will not be kept on the desired surface. If it is intended to measure cracks, fractures or micro-channels a low viscosity compound is preferable.
      2. Curing Time: The time the replication compound requires to solidify will depend on the specific compound in use and the application temperature. There are compounds with different curing velocities to facilitate its use at different temperatures. The curing time ranges from 2 to 60 minutes.
      3. Colors: A different coloring eases its sampling, collection and measurement.
      4. Special types: Special compounds are developed which can be applied under a wide range of temperatures or even under water conditions for corrosion, wear or damage inspection.

 

Shape measurement using Replication Compounds

The replication compounds can be used in the micro and macro scales. Viscosity plays an important role when capturing the shape of a component. Replication compounds suppliers usually have special pastes for that. Highly viscous polymeric plastelines are available with the same working principle. No dispenser pistol or nozzle is generally needed for those. The mixing of the polymers and its application is manually done.

 

Replication Compounds Accuracy

The accuracy of such replicas is generally set to 0.1 µm by the product manufacturers. The author did a rough benchmark tests to check its accuracy under different surface roughness on metal surfaces. A confocal microscope and different lenses were used for the following measurements:IMG_0010

Comparison Ra REFERENCE (Ra) – Ra REPLICA (Ra*)
Ra-Ra* (µm) (Ra-Ra*)/Ra (%)
50X 100X 150X 50X 100X 150X
N2 -0,286 0,036 0,03 -325,0% 34,0% 40,0%
N3 0,136 0,03 -0,017 53,5% 22,4% -12,4%
N6 0,18 -0,033 -0,023 29,6% -6,2% -6,1%
N7 0,351 -0,0273 0,028 29,2% -2,9% 3,1%
AVERAGE 0,09525 0,001425 0,0045 -53,2% 11,8% 6,1%

The results show a better accuracy than the one specified by the manufacturer. The so called “clear surface layer” is a translucent top surface film found in some replication compounds. This layer generates a certain ambiguity since it is not clear whether the microscope focuses on the top or the bottom of such layer. This phenomenon was not observed when doing this test.

A much accurate publication approaching this issue is found in this paper.

 

Cost of the Replication Kit and Compound Cartridges

The cost varies depending on the supplier and the volumes purchased. The following table shows some indicatives prices:

Quantity Item Cost
1 50 ml Manual dispensing gun 100 €
1 50ml Compound cartridge 60 €
10 Mixing nozzle 25 €

  •  
  •  
  •  
  •  
F. Xavier Borras
About F. Xavier Borras 6 Articles
Managing Editor, PhD Researcher & Founder of TriboEngineering

3 Comments

  1. Nice piece! Good to make people aware of this. As it is sometimes a forgotten technology. We use this almost on a daily basis to track the surface evolution of a surface in wear experiments. We came to the same conclusions when comparing the surface statistics. Next to that the absolute error between replica and real surface when subtracting the same areas was also very low.

  2. Hi dude, Im quite loving writings on your blog. They are structured properly, easy to consume and understand, in spite of English being my 3rd language. Cheers.

Leave a Reply to Charles Cancel reply

Your email address will not be published.


*


This site uses Akismet to reduce spam. Learn how your comment data is processed.